TABLE 1 - TYPICAL PROPERTIES SEALABLE TO MATERIALS 
SEALING GLASS REFERENCE GUIDE

Sealant ID
New ID   Old ID

 Exp.             Cont
(0-300C)(AP-25C)
      (x 10-7/C)

Density
(gm/cc)

AP SP
C C

Recommended
Sealing Cycle

Temp(C)

Time(min)

Max. Re-Heat
Temp(C)

            Sealable To:
 

Non-Metals

Metals

 SCY-1

RZ-1

3.5 10
2.59
638 ND
1200 20

    725

Quartz

SCY-2 RZ-2
5 10
2.70
570 ND
1200 20

    725

Quartz
SCE-3 SC-155
33 42
2.57
819 1070
1300 30

1055

Silicon
SCC-7 CV-635
36 48
3.90
- -
690 60

800

Silicon Carbide Molybdenum
SCQ-2 EN-9
38 52
2.86
685 870
1060 30
855
Aluminum Nitride
SCY-3 EZ-1
43 56
2.59
707 912
1120 30
895
Molybdenum

SCE-1

EE-2
43 56
2.59
765 960
1150 30
940
Molybdenum

SCB-1

SG-7

44 60
4.07
477 589
620 30
580
F15
SCR-2 SC-145
49 62
2.28
510 710
760 30
695
F15, Molybdenum
SCC-5 SC-950
51 70
4.07
- -
640 50
850
Alumina, Beryllia
SCQ-1 EN-4
52 76
2.51
570 723
970 30
705
Alumina, Beryllia F15, Molybdenum, Tantallm
SCQ-3 SC-150
56 71
2.32
520 710
760 30
700
Alumina F15, F30
SCQ-4 S-10000
59 78
2.41
575 752
1000 30
730
Alumina F15
SCG-1003 SC-136
59 80
ND
437 535
620 30
520
Alumina, Beryllia
SCC-2 CV-96
76 80
6.00
- -
450 30
525
Alumina, Beryllia F15, F30 (46%) F30 (42%)
SCB-2 SG-67
81 102
5.41
365 450
470 20
425
Ferrite, Fosterite F30 (52%), F31
SCC-1 CV-97
83 89
6.30
- -
460 60
525
Beryllia F31, Platinum, Titanium
SCC-3 CV-135
87 95
6.05
- -
435 60
550
Beryllia, Fosterite F31, F29, F30 (52%)
SCK-1 SC-105
90 103
2.67
447 680
950 30
645
Ferrite F30 (52%)
SCM-1 TM-5
90 107
2.68
456 655
930 20
640
Ferrite F256
SCB-3 SG-68
90 115
5.90
348 412
450 30
395
Ferrite F31, Platinum, Titanium
SCC-4 SC-900
95 100
6.53
- -
425 60
500
F30 (52%), F31
SCS-11 S-10005
97 139
2.51
466 557
650 30
545
Ferrite
*SCC-9 CC-10
99 104
6.48
- -
425 60
450
F256
SCL-1 TL-2
99 119
2.60
495 685
900 30
670
Ferrite
*SCC-10 CC-11
102 108
6.47
- -
425 60
450
F256
SCC-6 SC-200
117 127
6.55
- -
365 30
450
Ferrite Iron, SS302, SS304
SCS-1 ES-5
118 160
2.61
390 485
640 30
450
Iron, Inconel
SCU-2 EU-3
119 147
2.64
470 601
750 30
580
Iron, Inconel
SCG-1005 EG-5
123 140
3.23
403 563
840 30
540
Iron
SCU-1 EU-2
149 176
2.67
440 556
700 30
540
Copper
SCJ-1 EJ-3
161 173
3.63
320 406
550 20
380
Copper, SS302, SS304

* Conductive Glasses

NOTES:
1.  For crystallizing glasses, the contraction coefficient is measured from the recommended sealing temperature to 25 C.
2.  The annealing point and the softening point apply only to the vitreous glasses.
3.  These temperatures can be tolerated for up to ten (10) minutes.
4.  ASTM Metal Designations:
     F-15        29% nickel, 17% cobalt, 53% iron (eg. KOVAR, RODAR, THERLO)
     F-29        Copper clad - 42% nickel, iron (eg. Dumet)
     F-30        Nickel-iron alloys - 42% nickel, 44% nickel, 46% nickel, 49% nickel, 52% nickel
     F-31        42% nickel, 5.5 - 6% chromium, balance iron (eg. Sylvania #4, Carpenter #425)
     F-256      18% chromium, 82% iron (eg. #430 alloy)
     F-257      28% chromium, 72% iron (eg. #446 alloy)